What are some common quality problems with seamless steel tubes?

Apr 01, 2026

Leave a message

I. Cracks
Cracks are one of the most dangerous defects in seamless steel tubes. They manifest as straight, spiral, or network-like cracks on the inner and outer surfaces of the tube. The crack ends are sharp, and some can penetrate the tube wall.

Causes: Subcutaneous porosity, inclusions, or compositional segregation in the tube blank; uneven heating leading to uneven surfaces; excessive rolling pressure or rapid cooling causing thermal stress cracking.

Impact: Significantly reduces pressure-bearing capacity and easily expands during use, leading to sudden rupture.

II. Folds
Folds refer to overlapping of metal on the surface of the steel tube, appearing as straight or spiral stripes, resembling creases, often continuous or discontinuous.

Causes: Existing scratches, abrasions, or folds on the raw material surface that have not been removed; excessively deep edges at the grinding point; improper piercing process parameters (such as severe wear of the mandrel) leading to abnormal metal flow.

Impact: Causes localized stress concentration, reduces fatigue strength and corrosion resistance, and easily develops into cracks under long-term operation.

III. Uneven Wall Thickness and Eccentricity: Refers to inconsistent wall thickness on the same cross-section of the steel pipe, with one side thicker than the other, and in severe cases, a "single-sided thin wall" phenomenon.

Causes: Bending of the mandrel, mandrel misalignment, uneven guide plate spacing during piercing; uneven heating temperature leading to differences in deformation resistance; mill centerline misalignment or improper roll gap adjustment.

Impact: Weakens overall pressure uniformity, affects assembly accuracy, especially prominent in hydraulic systems and precision equipment.

IV. Inner Folding: Inner folding appears on the inner surface of the steel pipe, presenting as a straight or serrated folding defect; in high-alloy steel pipes, it often appears as an irregular block.

Causes: Excessive mandrel reduction before piercing; severe mandrel wear; looseness or segregation in the center of the billet; caused by alternating stress on the metal during piercing.

Impact: Reduces the smoothness of the inner wall, affecting media flow, and in severe cases, becomes a crack initiation point, leading to premature failure.

V. Scabs & Peeling
Scabs are thin, flaky metallic deposits adhering to the surface of the steel pipe. Peeling is the localized separation of metal from the substrate, appearing as nail-like bulges.

Causes: Impurities or iron oxide scale clumps in the lubricant; poor quality mandrels that are easily broken, with residue pressed into the inner wall; detached rear end lugs of the rough pipe pressed into the surface.

Impact: Damages surface integrity, making it prone to detachment during subsequent processing or use, forming pits, inducing corrosion or stress concentration.

VI. Matte Surface & Pitting
Matte surface refers to large areas of uneven, fine pits on the surface of the steel pipe, while pitting refers to periodic or locally distributed point defects.

Causes: Rough roll surface or iron oxide scale adhering to it; excessive pickling causing pinhole corrosion; unmelted glass lubricant or excessively low preheating temperature.

Impact: Reduces surface smoothness, affects coating adhesion, and easily induces pitting corrosion in humid environments.

VII. Scratches & Grooves: Scratches appear as spiral or straight groove-like defects on the steel pipe surface, sometimes with the groove bottom visible.

Causes: Wear or sticking of guide plates and exit nozzles; uneven roller surface; mechanical damage during transportation.

Impact: Creates stress concentration points, accelerating the corrosion process, especially in cold drawing, potentially developing into cracks.

VIII. Straightening Dents and Rolling Bending:

Straightening Dents: During straightening, excessive reduction or improper roll angle adjustment results in relatively smooth spiral-shaped dents on the steel pipe surface.

Rolling Bending: During rolling, metal enters the gap between the rolls or the tube becomes unstable, forming localized bulges or wrinkles, with the outer wall concave and the inner wall convex.

Impact: Affects appearance quality and dimensional accuracy; in severe cases, reduces structural strength. It is not permitted in qualified products.

IX. Other Defects:
Hairline Cracks: Fine, hair-like lines on the surface, caused by subcutaneous pores or inclusions in the tube blank; an early form of cracking.

Delamination: Delamination cracks appear in the tube wall, originating from non-metallic inclusions or shrinkage cavities; in severe cases, it leads to tube rupture.

Bulging (Convex Surface): Regular bulges on the outer surface, usually caused by pitting or depressions on the roll surface.

2025 Best 10 C45 Chromed Rod Suppliers in The World